高铝耐火制品
|
|
项目指标
|
Al2O3
%
≥
|
Fe2O3
%
≤
|
Zr2O
%
|
耐火度
℃
≥
|
显气孔率
%
≥
|
体积密度
g/cm3
≥
|
常温耐压
强度Mpa
≥
|
0.2Mpa荷重软化开始温度℃≥
|
重烧线
变化%
|
热震
1100℃水冷/次≥
|
|
电炉顶用高铝砖
|
|
DL-80
|
80
|
|
|
1790
|
19
|
|
78.5
|
1530
|
0-0.3
|
|
|
DL-75
|
75
|
|
|
1790
|
19
|
|
68.6
|
1530
|
0-0.4
|
|
|
高炉用高铝砖
|
|
DL-65
|
65
|
2.0
|
|
1790
|
19
|
|
58.8
|
1500
|
0-0.2
|
|
|
DL-55
|
55
|
2.0
|
|
|
19
|
|
49.0
|
1480
|
0-0.2
|
|
|
DL-48
|
48
|
2.0
|
|
|
18
|
|
49.0
|
1450
|
(1450℃×2h)0-0.2
|
|
|
抗剥落高铝砖
|
|
KBL-75
|
75
|
|
5-7
|
|
23
|
2.6
|
50
|
1500
|
|
20
|
|
KBL-70
|
70
|
|
5-7
|
|
25
|
2.55
|
45
|
1470
|
|
20
|
|
低蠕变高铝砖
|
|
DRLZ-80
|
85
|
|
|
|
20
|
|
60
|
|
(1550℃)0.8
|
|
|
DRLZ-75
|
75
|
|
|
|
20
|
|
55
|
|
(1550℃)0.8
|
|
|
DRLZ-65A
|
65
|
|
|
|
19
|
|
50
|
|
(1450℃)1.0
|
|
|
DRLZ-65B
|
65
|
|
|
|
22
|
|
45
|
|
(1400℃)0.8
|
|
|
DRLZ-60
|
60
|
|
|
|
22
|
|
40
|
|
(1300℃)0.8
|
|
|
DRLZ-50
|
50
|
|
|
|
22
|
|
40
|
|
(1250℃)0.8
|
|
|
硅莫砖
|
耐磨性≥
|
导热系数w/m·k
|
|
AZM-650
|
60
|
|
|
1790
|
20
|
2.55
|
90
|
1600
|
10cm3
|
2.5
|
|
AZM-1680
|
65
|
|
|
1800
|
19
|
2.60
|
85
|
1650
|
12cm3
|
2.3
|
|
|
|
|
|